Compare / E350 vs S355

E350 vs S355

India IS 2062:2011 · Steel

E350

Indian structural grade: 350 MPa yield, 490 MPa tensile, 22 % elongation.

Europe EN 10025-2:2019 · Steel

S355

Europe's workhorse structural steel: 355 MPa minimum yield up to 16 mm, 470–630 MPa tensile from 3 to 100 mm.

ApproximateYield 350 MPa for the thinnest band, 5 MPa below S355; minimum tensile 490 MPa, above S355's 470.

Mechanical

PropertyConditionE350S355Difference
Tensile strength Rmt = 3 mm≥ 490MPa1510–680MPa3+4.1 %
t = 100 mm≥ 490MPa1470–630MPa5−4.1 %
t = 150 mm≥ 490MPa1450–600MPa2−8.2 %
t = 250 mm≥ 490MPa1450–600MPa1−8.2 %
t = 400 mm≥ 490MPa1450–600MPa1−8.2 %
Elongation after fracture At = 40 mm≥ 22%1≥ 22%1same
t = 63 mm≥ 22%1≥ 21%1−4.5 %
t = 100 mm≥ 22%1≥ 20%1−9.1 %
t = 150 mm≥ 22%1≥ 18%—−18 %
t = 400 mm≥ 22%1≥ 17%—−23 %

Rows are matched by condition (thickness band, temperature, product form). A dash means the grade has no sourced value for that condition. Differences are S355 relative to E350; for ranges the lower bound is compared.