EuropeEN 485-2· Europe

5754-H24

Half-hard AlMg3 sheet and plate: 160 MPa proof, 240 MPa tensile up to 25 mm; welding drops the proof to 100 MPa.

Eurocode 9 gives H14 the same tensile with a higher proof (190 MPa) and lower elongation (3 %).

0.2 % proof strength Rp0.2
≥ 160MPa
From the standard≤ 25 mm
Tensile strength Rm
≥ 240MPa
From the standard≤ 25 mm
Elongation after fracture A
≥ 6%
From the standard≤ 25 mm · A50 or A as in Table 3.2a
Characteristic proof strength fo
160MPa
From the standard≤ 25 mm
Characteristic ultimate strength fu
240MPa
From the standard≤ 25 mm
HAZ proof strength fo,haz
100MPa
From the standard≤ 25 mm
HAZ ultimate strength fu,haz
190MPa
From the standard≤ 25 mm

All values

Mechanical

Strength

0.2 % proof strength Rp0.2

ConditionValueEvidence
≥ 160MPaFrom the standard

Tensile strength Rm

ConditionValueEvidence
≥ 240MPaFrom the standard

Ductility

Elongation after fracture A

ConditionValueEvidence
≥ 6%From the standard

Design values

Characteristic proof strength fo

ConditionValueEvidence
160MPaFrom the standard

Characteristic ultimate strength fu

ConditionValueEvidence
240MPaFrom the standard

HAZ proof strength fo,haz

ConditionValueEvidence
100MPaFrom the standard

HAZ ultimate strength fu,haz

ConditionValueEvidence
190MPaFrom the standard

Sources here are public pages that reproduce EN 485-2. For design and acceptance, the standard edition named in your specification and the inspection certificate (EN 10204 3.1) of the delivered product take precedence. Design factors are recommended values; your National Annex may set others.