C90/105

90 MPa cylinder, 105 MPa cube characteristic strength at 28 days; Ecm 44 GPa.

High-strength concrete: the strain limits εcu fall with strength, so the section is less ductile; Eurocode 2 adds rules above C50/60.

All values

Mechanical

Elastic

Secant modulus of elasticity Ecm

ConditionValueEvidence
44 000MPaCorroborated

Poisson's ratio ν

ConditionValueEvidence
0.2Single source

Strength

Characteristic cylinder strength fck

ConditionValueEvidence
90MPacharacteristicConfirmed

Characteristic cube strength fck,cube

ConditionValueEvidence
105MPacharacteristicConfirmed

Mean compressive strength fcm

ConditionValueEvidence
98MPaConfirmed

Mean axial tensile strength fctm

ConditionValueEvidence
5MPaCorroborated

Characteristic tensile strength (5 % fractile) fctk,0.05

ConditionValueEvidence
3.5MPacharacteristicCorroborated

Characteristic tensile strength (95 % fractile) fctk,0.95

ConditionValueEvidence
6.6MPacharacteristicCorroborated

Ductility

Strain at peak stress εc1

ConditionValueEvidence
2.8‰Corroborated

Ultimate strain (analysis curve) εcu1

ConditionValueEvidence
2.8‰Corroborated

Strain at maximum stress (parabola-rectangle) εc2

ConditionValueEvidence
2.6‰Corroborated

Ultimate strain (parabola-rectangle) εcu2

ConditionValueEvidence
2.6‰Corroborated

Exponent of the parabola n

ConditionValueEvidence
1.4Corroborated

Strain at maximum stress (bilinear) εc3

ConditionValueEvidence
2.3‰Corroborated

Ultimate strain (bilinear) εcu3

ConditionValueEvidence
2.6‰Corroborated

Design values

Long-term coefficient on compressive strength αcc

ConditionValueEvidence
1Single source

Partial factor for the material γc

ConditionValueEvidence
1.5Single source

Physical

Unit weight γ

ConditionValueEvidence
25kN/m³Single source

Thermal

Coefficient of thermal expansion α

ConditionValueEvidence
10×10⁻⁶ /KSingle source

Compare side by side

With any other grade

Sources here are public pages that reproduce EN 1992-1-1:2004. For design and acceptance, the standard edition named in your specification and the conformity evaluation of the delivered concrete (EN 206) take precedence. Design factors are recommended values; your National Annex may set others.