300W vs S275
CSA G40.21 · Steel
Canada's most common merchant structural grade: 300 MPa (44 ksi) yield, 65–90 ksi tensile.
EN 10025-2:2019 · Steel
Structural steel with 275 MPa minimum yield up to 16 mm, 410–560 MPa tensile.
ApproximateYield 300 MPa (44 ksi), above S275; tensile 450–620 MPa. 44W is the imperial name.
Mechanical
| Property | Condition | 300W | S275 | Difference |
|---|---|---|---|---|
| Yield strength ReH | t = 16 mm | ≥ 300MPa1 | ≥ 275MPa3 | −8.3 % |
| t = 40 mm | ≥ 300MPa1 | ≥ 265MPa3 | −12 % | |
| t = 63 mm | ≥ 300MPa1 | ≥ 255MPa2 | −15 % | |
| t = 63.5 mm | ≥ 300MPa1 | ≥ 245MPa2 | −18 % | |
| t = 80 mm | ≥ 275MPa1 | ≥ 245MPa2 | −11 % | |
| t = 100 mm | ≥ 275MPa1 | ≥ 235MPa2 | −15 % | |
| t = 101.6 mm | ≥ 275MPa1 | ≥ 225MPa2 | −18 % | |
| Tensile strength Rm | t = 3 mm | 450–620MPa1 | 430–580MPa1 | −4.4 % |
| t = 100 mm | 450–620MPa1 | 410–560MPa3 | −8.9 % | |
| t = 150 mm | 450–620MPa1 | 400–540MPa1 | −11 % | |
| t = 250 mm | 450–620MPa1 | 380–540MPa1 | −16 % |
Rows are matched by condition (thickness band, temperature, product form). A dash means the grade has no sourced value for that condition. Differences are S275 relative to 300W; for ranges the lower bound is compared.