Matipedia
EuropeEN 10151· Europe

1.4310

Austenitic spring stainless: 600 MPa annealed, cold rolled to 1 300–2 200 MPa for springs and spring clips.

Strength comes from cold rolling, which also makes it slightly magnetic. EN 10151 orders strip by tensile class (+C850 to +C1900); the guaranteed ranges of each class are not yet sourced here.

0.2 % proof strength Rp0.2
≥ 250 MPa1guaranteed minimum · annealed (solution treated), cold rolled strip
Tensile strength Rm
≥ 600 MPa1guaranteed minimum · annealed (solution treated), cold rolled strip
Density ρ
7 900 kg/m³1nominal
How we know these values · 13 values from 2 sources
Single source
13
  • Click any value under “All values” to see the sources that state it, with dates.
  • How we rate evidence

All values

Mechanical

Strength

0.2 % proof strength Rp0.2

ConditionValueEvidence
≥ 250MPaSingle source

Tensile strength Rm

ConditionValueEvidence
≥ 600MPaSingle source
≈ 750MPatypicalSingle source
≈ 1 350MPatypicalSingle source
≈ 1 900MPatypicalSingle source

Ductility

Elongation after fracture A

ConditionValueEvidence
≥ 40%Single source
≈ 45%typicalSingle source
≈ 10%typicalSingle source
≈ 0.5%typicalSingle source

Physical

Density ρ

ConditionValueEvidence
7 900kg/m³Single source

Thermal

Coefficient of thermal expansion α

ConditionValueEvidence
16×10⁻⁶ /KSingle source

Specific heat capacity cp

ConditionValueEvidence
500J/(kg·K)Single source

Thermal conductivity λ

ConditionValueEvidence
15W/(m·K)Single source